How to Choose Pigment Dispersions for DTF & DTG Textile Inks
A cyan can look strong on a film proof and weak on a black cotton shirt. Before changing the pigment, print a white-only patch alongside the cyan. In direct-to-film (DTF) production, the backing, adhesive and transfer determine what the customer sees. In direct-to-garment (DTG) printing, the same colour is affected by the fabric surface, pretreatment and ink fixation. The most revealing comparison is a pair of finished garments printed under controlled conditions.
Which parts of the trial change between DTF and DTG?
| Where to look | Conventional powder-based DTF | DTG on cotton |
|---|---|---|
| Where the drop lands | Print colour onto the coated side of the same release film. Check for pooling, coalescence and loss of detail before adding the white backing. | Use the same knit, dye lot and fabric finish. Check whether fine lines spread along the yarns or fibres protrude through the printed surface. |
| White underbase | Hold white ink and laydown constant behind the colour layer. Judge a white-only patch and the colour patches after transfer onto the intended dark garment. | On dark cotton, fix the pretreatment as required and print the same white underbase before CMYK. Record pretreatment mass per unit area and white coverage. Include a light-cotton control if the intended process also prints without an underbase. |
| What holds the print | Use the same powder lot and application, adhesive melt conditions, press settings and peel procedure. Examine fine edges and solid areas after peeling. | The ink binder has to form a durable film on the fibres. Record the cure method, time and temperature reached at the print. Check rub-off and fibre exposure after washing. |
Epson’s F2270 film instructions tie the transfer settings to the film, powder, equipment and ink laydown. Brother’s GTX instructions describe how an evenly applied pretreatment supports a white layer on dark fabric and a surface for the colour overprint. Use the instructions specific to the system under test. Epson film post-processing · Brother GTX pretreatment guidance.
Which grade deserves a formulation trial?
Set a target shade on an agreed fabric first. For a process-colour set, AIC lists Cyan 6900 (PB15:3), Magenta Pink K6B (PV19), Yellow 2024 (PY155) and Black 0058 (PBk7). All four are aqueous carboxylic dispersions with a nominal pigment loading of 15 wt%. Compare candidates at equal pigment loading in the intended binder and vehicle. For magenta, print a solid patch and red and blue overprints so that a good single-colour match does not hide a shift in the mixed colours. Compare all four grades, their technical sheets and sample options.
AIC-Black 0058 is one example. Its published sample has D50 of 127 nm and D90 of 172 nm. These values help identify the material entering the trial. After adding the binder and humectants, check the finished ink’s viscosity at the intended head temperature, filtration and nozzle recovery after idle time. Then compare black density on the finished garment at matched ink laydown. Black 0058 product data · Original particle-size report.
How much white gives enough coverage without a stiff print?
Make a short white-laydown series on the target dark garment, using one colour recipe throughout. Include a white-only patch, a full-colour solid and a fine-detail motif at each setting. Record white-patch lightness (L*) using the same instrument settings and backing. Compare the overprinted colours against the approved garment. Fold, stretch and release equal-sized printed areas alongside the reference, then ask assessors to compare stiffness and surface feel with the samples coded. Record the lowest white laydown that meets both the appearance and hand targets.
For white-ink development, AIC-WHITE S701 is an evaluation grade. Confirm sample availability with AIC. Its TDS describes the dispersion. A garment trial supplies the evidence for underbase coverage, flexibility and wash performance. For storage, also record the idle time and temperature, sediment remaining after the agreed mixing procedure, and which nozzles recover on restart. S701 development status and TDS.
How should the buyer assess washing and rubbing?
Run the candidate and the approved reference on matched garments. Retain an unwashed panel from each print. Record the time between finishing and testing. In DTG, incomplete fixation can cause colour loss in washing or rubbing, so compare the cure record before attributing a failure to the pigment. Epson guidance on ink fixation.
- Wash fastness. For a laboratory comparison of colour change and staining, agree the applicable ISO 105-C06 procedure with the customer. Record the procedure and assess the printed specimen and adjacent fabric separately. ISO 105-C06.
- Repeated garment washing. For a claim about repeated home laundering, define the wash and dry programmes, detergent, temperature and number of complete cycles. Photograph the same areas after each agreed interval. Score DTF cracking and edge lift separately from colour change. For DTG, inspect colour loss, newly exposed fibres and areas of white showing through the colour. ISO 6330 washing and drying procedures.
- Dry and wet rubbing. Report staining of the rubbing cloth under each condition. A garment can retain its apparent shade yet transfer colour when rubbed. Agree the minimum acceptable ratings with the buyer before comparing samples. ISO 105-X12.
If both DTF samples lift at the same edges, repeat the transfer with the approved film and verified press conditions. If both DTG samples wash down where the white layer was uneven, check pretreatment uniformity and fixation. When the reference passes and only the candidate fails, repeat the comparison on a second print run with the same formulation and substrate controls before qualifying the grade.