Formulating High-Speed Single-Pass Corrugated Packaging Inks: Phosphate vs. Carboxylic Pigment Dispersions

For a single-pass corrugated packaging line targeting 60–150 m/min, the ink needs to keep pigment dispersed through the printbar and immobilise it quickly on the liner. Screen self-dispersed colourants in the complete ink to reduce agglomeration and nozzle deposits on piezo printheads such as Kyocera KJ4B, Ricoh Gen5/Gen6 or Fujifilm Dimatix SAMBA. Pair that screening with trials on the actual kraft liner and primer to control feathering and intercolour bleed. Start with two 15 wt% PB15:3 cyan dispersions at equal pigment loading, then compare filterability, nozzle restart, optical density and dry rub at the intended line speed.

Why fast jetting and sharp print are separate tests

Uncoated kraft liners can pull pigment away from the surface

When a drop strikes uncoated kraft, the vehicle enters the pores and can spread along the fibres. If too much pigment follows it below the surface, solid patches can lose optical density and fine edges can feather. Brown liner colour also changes the appearance of the print. Compare the same image on the same liner lot at equal ink laydown. Measure dry density and CIELAB colour alongside line width and bleed between adjacent colours. Keep the paper reference, measurement geometry and backing consistent.

Drying time shrinks as line speed rises. With 3 m of effective dryer length, the dwell time drops from 3.0 seconds at 60 m/min to 1.2 seconds at 150 m/min. Commercial aqueous presses illustrate this range. Xeikon lists 60–120 m/min for IDERA. Hanway lists 75–150 m/min for the standard Glory2504. Run trials within the ratings for your press and board, using the actual dryer length, air settings and coverage. Xeikon IDERA specifications · Hanway Glory2504 specifications (PDF)

Calcium and magnesium are helpful on some liners and disruptive in the ink circuit

Calcium and magnesium can screen the charge on dispersed particles. In the ink circuit, that can encourage flocculation, reduce filter throughput and disturb jetting. On an appropriately treated liner, rapid immobilisation after impact can keep more pigment near the surface. Paper studies have observed this effect for specific ink and salt combinations. Keep any primer separate from the ink circuit and compare it against the same untreated liner. A calcium-rich primer can change the result even when the base paper and the ink are the same. Oko et al., study of calcium and magnesium in pigment ink–paper interactions

High-frequency printbars need a viscosity window for the finished ink

At high duty cycles, micron-scale nozzle channels must refill between firings. AIC’s ≤3 mPa·s TDS limit applies to the concentrates in the table. It gives the formulator room to add binder and humectants. The finished ink must match the selected head’s viscosity and surface-tension window at the actual jetting temperature. Kyocera lists 5.0–6.0 mPa·s for selected KJ4B models, including the KJ4B-EX1200-RC. Ricoh lists 10–12 mPa·s for the MH5420/5440 and MH5320/5340 under its reference test conditions. Fujifilm Dimatix lists 4–8 mPa·s for SAMBA G3L and 5–9 mPa·s for SAMBA G5L for highest performance. Check the full model designation and the integrator’s fluid limits before trialling. Kyocera product lineup · Ricoh MH5420/5440 · Ricoh MH5320/5340 · SAMBA G3L/G5L data sheet (PDF)

When a piezo head develops missing or deflected jets, look for dried ink on the nozzle plate, agglomerates, trapped air and poor nozzle-face wetting. In thermal inkjet, kogation specifically describes deposits on a firing resistor. That distinction helps the team choose the right diagnostic test for the head it is running. Halko, thermal inkjet kogation study

CMYK concentrate specifications for a corrugated ink trial

Start with the two cyan grades. They share the same Colour Index, PB15:3, and 15 wt% nominal pigment content. Their carboxylic and phosphate surface groups give the formulator two ways to tune how the pigment responds to pH, the binder and dissolved ions. Compare the grades in an otherwise matched vehicle, using the planned production water. Hold finished-ink pigment loading, binder solids, pH and laydown constant. Check the same ink before and after ageing, then test it against the actual liner and primer at press speed.

Five AIC self-dispersed aqueous concentrates as supplied. D50 values link to individual sample reports.
AIC gradeColour IndexSurface chemistryNominal pigmentTDS viscosity (mPa·s)Sample D50 (nm)Data sheet
AIC-Cyan HC-7533PB15:3Phosphate15 wt%≤3157TDS (PDF)
AIC-Cyan 6900PB15:3Carboxylic15 wt%≤3141TDS (PDF)
AIC-Magenta Pink K6BPV19Carboxylic15 wt%*≤3145TDS (PDF)
AIC-Yellow 2024PY155Carboxylic15 wt%≤3136TDS (PDF)
AIC-Black 0058PBk7Carboxylic15 wt%≤3127TDS (PDF)

*K6B’s nominal pigment content is published on its product page. The 127–157 nm D50 range describes the five individual samples. For HC-7533, the sample measured 157 nm and the TDS lists a separate indicative target of ≤150 nm. For incoming approval, agree the test method and acceptance limits and review the current lot COA.

D50 describes the median of the measured distribution. After adding the binder and humectants, check D90 and D97 as indicators of the coarse tail and time equal sample volumes through the same membrane under fixed conditions. A few agglomerates can shorten filter life even when D50 barely moves. Compare with the qualified reference before and after storage and record filter residue, pH and conductivity. AIC particle-size report library · Interpreting particle-size data

Four checks before qualifying the ink for production

  1. Drying, density and edge quality. Print solid CMYK patches, heavy overprints, fine lines and reverse type on the intended kraft and coated grades. At the stacker or transfer point, check set-off by pressing a clean sheet against the print under a defined load and time. After conditioning, measure density, colour and edge spread. Test at normal speed and the fastest planned setting, holding coverage, laydown and measurement conditions constant. An ink that looks dry may still transfer to the next sheet in the stack.
  2. Dry rub and scuff resistance. Condition the printed board for an agreed interval. Use a defined counterface, load and cycle count, following ASTM D5264 when specified by the buyer. Record transfer to the receptor, density loss and visible damage. Separate colour transfer from fibre tear or varnish failure. Test wet rub separately if required by handling or end use. ASTM D5264, printed-material abrasion testing
  3. Decap time and high-duty nozzle recovery. Establish an active-nozzle baseline at the prescribed jetting temperature. Run a representative high-coverage pattern, then introduce uncapped pauses relevant to the line and permitted by the integrator. During a pause, selective evaporation can change the ink composition at the nozzle exit. Log first-pass active nozzles as a percentage of the baseline, along with deflected jets, streaks and the time or purge cycles needed to return to normal. Record humidity, printhead temperature and recirculation settings. Use the longest pause that still meets the agreed restart criteria as the working decap time for that setup. Rump et al., study of evaporation at piezo nozzles
  4. Batch release and supply qualification. Review the incoming grade’s TDS and SDS, and request a lot-specific COA. Agree which properties are release criteria for both the concentrate and the finished ink. AIC’s production site in Linyi, Shandong, China, covers 5,000 m² and has a stated full production capacity of 120 metric tonnes per month. Bulk formats are 25 kg or 200 kg per container, or 1,000 kg per IBC. The AIC supplier statement lists EU REACH references for the selected pigment substances, including PB15:3, PV19, PY155 and PBk7. Confirm coverage for your grade and supply chain. Türkiye KKDIK registration work is in progress. Review any food-contact, migration or set-off requirements for the finished packaging separately. AIC production capabilities · Pigment-substance registration statement · Sample and bulk formats

Frequently asked questions

What is the advantage of phosphate groups in a corrugated pigment ink?

Phosphate groups give formulators another way to tune how an anionic pigment interacts with binders and dissolved ions. Compare phosphate and carboxylic PB15:3 at the same pigment loading. A useful grade remains stable in the ink circuit and gives the required density and edge quality on the target liner or primer. Salt tolerance depends on the whole ink vehicle.

Can I use these dispersions with Kyocera KJ4B, Ricoh Gen5 or Gen6, or Fujifilm Dimatix SAMBA?

Use the grades as raw materials when developing an aqueous ink for the exact head model and press. Check the integrator’s limits for the complete ink at jetting temperature, then verify drop formation, filter loading, nozzle recovery and sustained firing on an approved test stand.

What sample and bulk packaging can I request?

Evaluation samples are 500 mL–1 L per bottle. Standard bulk formats are 25 kg or 200 kg per container, or 1,000 kg per intermediate bulk container (IBC). Request the grade-specific TDS and SDS and the COA for the evaluation or supply lot.

Request samples for a single-pass corrugated ink trial

Tell us the printhead model, target speed, liner and any primer or varnish. Request 500 mL–1 L per sample bottle, the grade-specific TDS and SDS, and the COA and available particle-size report for the evaluation lot.

Browse the Product Center · Find grades for corrugated printing